Yangjiazhangzi beneficiation plant: Yangjiazhangzi processing plant was built in 1966, a wet workshop, molybdenum ore processing, production of industrial ammonium.
Ammonium molybdate production process:
1) Sodium hypochlorite leaching: reaction formula
MoS2+9NaClO+6NaOH→Na2MoO4+Na2SO4+9NaCl+3H2O
2) Calcium molybdate precipitation: adjust the pH to 5~6 with hydrochloric acid, add CaCl2, boil with steam, and precipitate calcium molybdate.
3) Soda leaching calcium molybdate: reaction formula
CaMoO4+Na2CO3↔Na2MoO4+CaCO3↓
4) Precipitated molybdic acid: hydrochloric acid is added to a pH of 0.5, the temperature is above 95 ° C, and the precipitation rate is generally above 95%.
5) Ammonia water dissolves molybdic acid: To accelerate the reaction, the dissolution should be carried out at a temperature of 70 to 80 °C.
6) Precipitating ammonium molybdate: Ammonium molybdate solution is added to hydrochloric acid at a temperature of 30 to 40 ° C to a pH of about 2.5 to precipitate a white crystal precipitate. The precipitation rate can reach more than 96%. After being dehydrated, dried and pulverized by a centrifuge, it is a finished product. The production process is shown in the following figure:
Share to:
Privacy statement: Your privacy is very important to Us. Our company promises not to disclose your personal information to any external company with out your explicit permission.
Fill in more information so that we can get in touch with you faster
Privacy statement: Your privacy is very important to Us. Our company promises not to disclose your personal information to any external company with out your explicit permission.